H111 |
Annealed and slightly strain-hardened (less than H11) during subsequent operations such as stretching or levelling. |
H112 |
Slightly strain-hardened from working at an elevated temperature from a limited amount of cold work (mechanical property limits specified). |
H114 |
Applies to embossed or patterned sheet or strip, fabricated from the corresponding Hxx temper. |
H12 |
Strain-hardened - 1/4 hard |
H14 |
Strain-hardened - 1/2 hard. |
H16 |
Strain-hardened - 3/4 hard. |
H18 |
Strain-hardened - 4/4 hard (fully hardened). |
H19 |
Strain-hardened - extra hard. |
H22 |
Strain-hardened and partially annealed - 1/4 hard. |
H24 |
Strain-hardened and partially annealed - 1/2 hard. |
H244 |
Applies to embossed or patterned sheet or strip, fabricated from the corresponding Hxx temper. |
H32 |
Strain-hardened and stabilized - 1/4 hard. |
H34 |
Strain-hardened and stabilized - 1/2 hard. |
H42 |
Strain-hardened and painted or lacquered - 1/4 hard. |
H44 |
Strain-hardened and painted or lacquered - 1/2 hard. |
O |
Annealed - products achieving the required annealed properties after hot forming processes may be designated as O temper. |
T1 |
Cooled from an elevated temperature shaping process and naturally aged. |
T3 |
Solution heat-treated, cold worked and naturally aged. |
T351 |
Solution heat-treated, stress-relieved by controlled stretching (permanent set 0.5% to 3% for sheet, 1.5% to 3% for plate, 1% to 3% for rolled or cold-finished rod and bar, 1% to 5% for hand or ring forging and rolled ring) and naturally aged. The products receive no further straightening after |
T3510 |
Solution heat-treated, stress-relieved by controlled stretching (permanent set 1% to 3% for extruded rod, bar, shapes and tube, 0.5% to 3% for drawn tube) and naturally aged. The products receive no further straightening after stretching. |
T4 |
Solution heat-treated and naturally aged. |
T451 |
Solution heat-treated, stress-relieved by controlled stretching (permanent set 0.5% to 3% for sheet, 1.5% to 3% for plate, 1% to 3% for rolled or cold-finished rod and bar, 1% to 5% for hand or ring forging and rolled ring) and naturally aged. The products receive no further straightening after stretching. |
T4511 |
Same as T4510 except that minor straightening is allowed after stretching to comply with standard tolerances. |
T5 |
Cooled from an elavated temperature shaping process and then artificially aged. |
T6 |
Solution heat-treated and then artificially aged. |
T651 |
Solution heat-treated, stress-relieved by controlled stretching (permanent set 0.5% to 3% for sheet, 1.5% to 3% for plate, 1% to 3% for rolled or cold-finished rod and bar, 1% to 5% for hand or ring forging and rolled ring) and then artificially aged. The products receive no further straightening after stretching. |
T6510 |
Solution heat-treated, stress-relieved by controlled stretching (permanent set 1% to 3% for extruded rod, bar, shapes and tube, 0.5% to 3% for drawn tube) and then artificially overaged in order to achieve a good exfoliation corrosion resistance. The products receive no further straightening after stretching. |
T6511 |
Same as T6510 except that minor straightening is allowed after stretching to comply with standard tolerances. |
T66 |
Solution heat-treated and then artificially aged - mechanical property level higher than T6 achieved through special control of the process (6000 series alloys). |
T7 |
Solution heat-treated and then artificially overaged. |
T73 |
Solution heat-treated and then artificially overaged in order to achieve the best stress corrosion resistance. |
T7351 |
Solution heat-treated, stress-relieved by controlled stretching (permanent set 0.5% to 3% for sheet, 1.5% to 3% for plate, 1% to 3% for rolled or cold-finished rod and bar, 1% to 5% for hand or ring forging and rolled ring) and then artificially overaged in order to achieve the best stress corrosion resistance. The products receive no further straightening after stretching. |
T7451 |
Solution heat-treated, stress-relieved by controlled stretching (permanent set 0.5% to 3% for sheet, 1.5% to 3% for plate, 1% to 3% for rolled or cold-finished rod and bar, 1% to 5% for hand or ring forging and rolled ring) and then artificially overaged (between T73 and T76). The products receive no further straightening after stretching. |
T8 |
Solution heat-treated, cold worked and then artificially aged. |
T9 |
Solution heat-treated, artificially aged and then cold worked. |